In the present study, the tribological properties of diverse crystalline diamond coating with micro (MCD) and nanometer (NCD) sizes, fabricated by the microwave plasma chemical vapor deposition (MPCVD) method, are systematically investigated in dry and seawater environments, respectively. Owing to the SiO2 lubricating film with extraordinary hydrophilicity performance by a tribochemical reaction, the average friction coefficient (COF) and wear rate of NCD coating under seawater decreased by 37.8% and 26.5%, respectively, comparing with in dry conditions. Furthermore, graphite would be generated with the increment of surface roughness. Graphite transformed from the diamond under high contact pressure. Thus, with the synergism between SiO2 lubricating film with extraordinary hydrophilicity performance and graphite, the corresponding COF and wear rate of MCD would be further decreased by up to 64.1% and 39.5%. Meanwhile, various characterizations on morphology, spectra, and tribological performance of the deposited diamond coating were conducted to explore the in-depth mechanism of the enhanced tribological performance of our NCD and MCD coatings in the extreme under seawater working conditions. We envision this work would provide significant insights into the wear behavior of diamond coatings in seawater and broaden their applications in protective coatings for marine science.